Received: April 04, 2025
Accepted: January 21, 2026
Available: February 16, 2026
Nanofluids with magnetic nanoparticles have been proposed to enhance heat transfer and energy conversion. However, the performance of these fluids depends on suspension stability and thermal distribution under irradiation. Low-frequency acoustic excitation emerges as an active strategy to modulate mixing and heat transport in these systems. The objective of this research was to determine the effect of low-frequency acoustic excitation on suspension stability, radiative absorption, and thermal efficiency of nanofluids containing magnetite nanoparticles (Fe₃O₄) dispersed at 0.05, 0.25, and 0.5% v/v in an ethylene glycol–water mixture. The methodology included exposing the nanofluids to acoustic waves generated by a loudspeaker while irradiating them with visible and infrared light from a halogen lamp. Stability was assessed through transmittance measurements, and thermal evolution and energy conversion were characterized using the specific absorption rate (SAR) and the stored energy ratio (SER). A comparison was made between different nanoparticle concentrations and excitation conditions. The results demonstrated that acoustic excitation influenced the stability and thermal distribution of the fluid. The extent of these effects varied depending on concentration and experimental conditions. In particular, excitation reduced thermal stratification and increased homogenization in certain cases, whereas in others it did not yield significant improvements in thermal efficiency (SAR/SER). Finally, it is concluded that when used in conjunction with an acoustic excitation system, nanofluids can be utilized more effectively in thermal applications because the acoustic excitation system promotes more uniform temperature fields.
Keywords: Acoustic wave, energy conversion, ferrofluid, nanoparticle, thermal energy.
Los nanofluidos con nanopartículas magnéticas se han propuesto para mejorar la transferencia de calor y la conversión energética; sin embargo, su desempeño depende de la estabilidad de la suspensión y de la distribución térmica bajo irradiación. La excitación acústica de baja frecuencia se perfila como una estrategia activa para modular la mezcla y el transporte de calor en estos sistemas. El objetivo de esta investigación fue determinar el efecto de una excitación acústica de baja frecuencia sobre la estabilidad de la suspensión, la absorción radiactiva y la eficiencia térmica de nanofluidos con nanopartículas de magnetita (Fe₃O₄) dispersas a 0,05; 0,25 y 0,5 % v/v en una mezcla de etilenglicol y agua. La metodología empleada consistió en exponer los nanofluidos a ondas acústicas generadas por un altavoz mientras se irradiaban con luz visible e infrarroja de una lámpara halógena. La estabilidad se evaluó mediante medidas de transmitancia, y la evolución térmica y la conversión de energía se caracterizaron mediante la tasa de absorción específica (SAR) y la razón de energía almacenada (SER). Se compararon las distintas concentraciones de nanopartículas y las condiciones experimentales de excitación. Los resultados mostraron que la excitación acústica modificó la estabilidad y la distribución térmica del fluido, y la magnitud de los efectos dependió de la concentración y del régimen experimental. En particular, la excitación redujo la estratificación térmica e incrementó la homogeneización en ciertos casos, mientras que en otros no produjo mejoras significativas en la eficiencia térmica (SAR/SER). Finalmente, se concluye que la incorporación de un sistema de excitación acústica puede optimizar el desempeño de los nanofluidos en aplicaciones térmicas al favorecer campos de temperatura más uniformes.
Palabras clave: Onda acústica, conversión energética, ferrofluido, nanopartícula, energía térmica.
Renewable energies have emerged as a sustainable solution, with solar energy representing a particularly promising avenue for mitigating environmental impacts and diversifying the energy matrix
Solar energy is harnessed through direct conversion to electricity using photovoltaic systems and heat capture using solar thermal collectors, which are used to heat fluids for heating applications and industrial processes
In Direct Absorption Solar Collectors (DASCs), the working fluids can range from common liquids, such as water, ethylene glycol, and oil, to advanced colloids, such as nanofluids
The settling of nanoparticles in working fluids alters their optical and thermal properties, which may subsequently reduce the efficiency of DASC systems. As the nanoparticles settle, the fluid loses its homogeneity, reducing its capacity to absorb and convert solar radiation into thermal energy in a uniform manner
The stability of nanofluids can be classified into two strategies: those associated with the formulation process and those related to operation. The formulation conditions include the use of surfactants such as some carboxylic acids, pH adjustment by the addition of acids or bases, and appropriate selection of agitation power
Similarly, the use of ultrasonic waves has been demonstrated to enhance the stability of nanofluids and influence the transfer of heat through the processes of cavitation and agitation, thereby promoting uniform mixing and preventing particle settling
In particular, in systems where the nanofluids under examination are confined, low-frequency waves induce a slight agitation in the fluid, which increases the Nusselt number by improving circulation and thermal transport in the areas near the surfaces. Moreover, the implementation of these waves causes alterations in the drag and lift coefficients, which promote vortex shedding in the nanofluid
This study aims to analyze how applying a low-frequency acoustic field enhances the ability of a nanofluid (Fe3O4/EG-H2O) to capture visible radiation energy. Specifically, it evaluates how variations in solid concentration, radiation, and mechanical waves influence the amount of captured energy converted into temperature. The experimental setup included an acoustical loudspeaker to agitate the fluid volume while exposing it to a visible-light radiation source, allowing for thermal monitoring of the sample. This setup provides a deeper understanding of how these operational variables affect the thermal performance of nanofluids, thereby helping to determine their potential applications in solar energy harvesting systems.
2.1 Preparation of samples
The ethylene glycol (EG) used in this study was procured from Panreac. A solution of water and ethylene glycol (1:1) was prepared as the base fluid. Subsequently, the quantities required for the preparation of 50 ml of nanofluids were determined at volumetric concentrations of 0.05%, 0.25%, and 0.5% Fe3O4, as defined in the review concerning the formulation of nanofluids applicable to solar collectors. Fe₃O₄ nanoparticles of diameter (50 to 100 nanometers) were used, and they were supplied by Merck.
The preparation of the suspensions involved calculating the necessary amounts of water, ethylene glycol, and Fe₃O₄ using the mixture rule. The calculations used the density and specific heat data from Table 1 to determine the required quantities (Table 2. After mixing the components, the process included 30 min of mechanical agitation, followed by 10 min of ultrasound homogenization at 400 W and 20 kHz using a TU-1000E4 (Xian Toption Instrument Co).
| Property | Unit | Water | Ethylene glycol | Water/EG 1:1 | Fe3O4 |
| Density | kg/m3 | 997 | 1115 | 1054 | 5200 |
| Specific Heat | J/kg°C | 4180 | 2430 | 3256 | 670 |
| Magnitude | Unit | Sample | ||||
| 0% | 0.05% | 0.25% | 0.5% | |||
| Liquid Volume | Vf | cm3 | 50 | 49 | 49 | 49 |
| Particle Volume | Vp | cm3 | 0.00 | 0.025 | 0.125 | 0.25 |
| Liquid Mass | mf | g | 52.800 | 52.904 | 53.318 | 53.836 |
| Particle Mass | mnp | g | 0.000 | 0.130 | 0.650 | 1.300 |
| Nanofluid density | ρnf | kg/m3 | 1056 | 1058 | 1066 | 1077 |
| Nanofluid-specific heat | Cpnf | J/kg.°C | 3256 | 3254 | 3248 | 3240 |
Table 2 presents the calculated properties for the evaluated samples, which varied according to the nanoparticle concentration. The density and specific heat are calculated using equations (1) and (2) In these equations, φ represents the percentage of the nanoparticle concentration, while 𝜌𝑏𝑓 and 𝜌𝑛𝑝 indicate the density of the base fluid and nanoparticle, respectively. Similarly, 𝐶𝑝,𝑏𝑓 and 𝐶𝑝,𝑛𝑝, correspond to the specific heats of the base fluid and nanoparticle, respectively
(1)
(2)
2.2 Nanofluids characterization
An XRD spectrum was obtained to identify the crystalline phases in the sample using a PANalytical Aeris instrument (PANalytical B.V.) with Cu-Kα as the X-ray source. The particle morphology and size were analyzed using images acquired with a Thermo Fisher Scientific Scios 2 LoVac dual-beam field emission scanning electron microscope (FIB-FESEM).
The stability of the nanofluids was evaluated using an A721 spectrophotometer. The samples were subjected to mechanical agitation for 10 min and subsequently deposited into acrylic cuvettes. Transmittance data for wavelengths between 350 and 1000 nm were collected at 5-minute intervals over a 30-minute period.
2.3 Experimental set-up
The samples were subjected to a 10-minute agitation process. Twenty-five milliliters of nanofluids were deposited on a glass Petri dish with a circular cross-sectional area of 3x10⁻³ m². The Petri dish was affixed to a loudspeaker using plastic cable ties to facilitate contact and transmission of mechanical excitation to the fluid. Furthermore, the sample was subjected to visible infrared radiation generated by a 250 W-60 Hz infrared lamp light bulb and a flat convex concentrator lens.
Figure 1 illustrates the experimental setup used to study the effects of simulated radiation and mechanical waves on a sample containing Fe₃O₄ magnetite nanoparticles. The setup includes a Máxima infrared lamp with a concentrator that directs light onto a 25 mL sample with nanoparticle concentrations of 0.5%, 0.25%, and 0.05% v/v. The lamp was preheated with a voltage of 110 V, power of 250 W, and frequency of 60 Hz for 10 min before exposure to ensure stable irradiance. A SM206-SOLAR pyranometer measured the power and recorded 1000 W/m² when the incident surface was 16 cm from the sample. Temperature monitoring was performed using a UT325 thermometer multimeter with type K thermocouples positioned at two depths in the liquid, 7 mm apart and 3.5 mm from the sample surface, to track temperature evolution throughout the experiment. In addition, a mechanical wave generator loudspeaker configured at 200 Hz introduced vibrations into the sample.
The experiment was conducted for a period of 10 min, during which the temperature of the two thermocouples was recorded at 60-s intervals. During this time, a 200-Hz and 45-dB square wave was generated by the loudspeaker. A frequency of 200 Hz and 45 dB used in the experiment were selected after oscillations were observed on the fluid surface, as shown in the subsequent results and discussion section. The surface oscillations indicate the generation of an agitation regime in the sample, which is associated with its composition and viscosity. This phenomenon suggests that the mechanical excitation at this frequency promotes forced convection in the nanofluid, thereby preventing the rapid sedimentation of the nanoparticles and homogenization in the thermal stratification of the sample.
2.4 Efficiency evaluation
To evaluate the performance of the heating system, the time evolution of the temperature was measured by the thermocouples. The temperature difference between the two thermocouples was calculated, as this provides information regarding the homogeneity of the thermal process of radiation transformation.
The specific absorption rate (SAR) and stored energy ratio (SER) were measured. The comparison between the SAR and SER values of different nanofluid formulations allows the determination of suspended solid concentrations that maximize the thermo-absorption effect. In addition, these indicators were used to evaluate operational variations due to the application of mechanical waves were analyzed, which allows evaluated whether of incident radiation transformed increases the internal energy in the nanofluid for the concentrations used.
The SAR is defined as the amount of energy captured by the nanofluid, normalized by the number of suspended solids present. This provides information about the efficiency of operating at a given concentration. The specific absorption rate (SAR) was calculated using the simplified mixing equation for a given nanofluid, as outlined in (3)
(3)
The specific heat data and masses of the substances were calculated as simple mixture properties from the volumetric concentrations of water, EG, and Fe3O4 and are reported in Table 1.The change average temperature data,
and
were the average of two thermocouples located in the fluid for each time interval Δt. Where
is the sample corresponding to the nanofluid and
is the sample corresponding to the base fluid. mnp is the mass in kilograms of the nanoparticles comprising the analyzed sample. Cpnf and Cpbf are the specific heats of the nanofluid samples, calculated based on their nanoparticle content and the specific heat of the base fluid, respectively, as shown in Table 1. The SAR is calculated temporally with a Δt=60 sec, in addition it is also calculated taking the whole experimental interval, which is Δt=600 sec.
The stored energy ratio SER, on the other hand, refers to the ratio of the energy stored by the nanofluid to the base fluid. The SER was calculated using the following in (4)
(4)
Where
and
represent the average temperatures of the nanofluid and base fluid at each time t, respectively.
and
being the temperature of the nanofluid and base fluid at time t=0.
Figure 2 shows the XRD spectra. The identified peaks are consistent with those expected for pure Fe₃O₄ samples, where 30.13°, 35.50°, and 43.15° correspond to the (220), (311), and (400) diffraction planes, respectively, related to the inverse spinel crystal structure with a lattice parameter of 8.396 Å.
Figure 3 shows images of Fe₃O₄ nanoparticles captured using a field emission scanning electron microscope (FIB-FESEM). The nanoparticles exhibit a variety of shapes, including cubic and rounded forms, resulting in a range of particle sizes. The tendency of these nanoparticles to cluster together suggests that the nanofluids may exhibit low stability because of gravitational effects acting on them. Furthermore, particles exceeding the size range specified by the supplier are evidenced, rendering them particularly susceptible to precipitation.
Figure 4 shows a visual representation of the four samples that were subjected to evaluation: the 1:1 mixture of water and ethylene glycol, as well as the Fe₃O₄ nanofluids at concentrations of 0.05%, 0.25%, and 0.5% v/v, which were prepared in accordance with the parameters outlined in Section 2.1.
As illustrated in Figure 5a, the behavior of the analyzed fluids is demonstrated in the wavelength range 350–1020 nm. The EG/H2O mixture maintains translucency across the entire spectrum, whereas the nanofluids at their three initial concentrations exhibit complete opacity to radiation within this range. Conversely, Figure 5b presents the time evolution of the transmittance at a wavelength of 550 nm, which was selected based on the reported transmittance peak for magnetite in the literature. The EG/H2O mixture exhibited stable behavior over time, consistent with its homogeneous nature and resistance to degradation.
Conversely, nanofluids with concentrations of 0.5% and 0.25% v/v exhibit increased transmittance, reaching 100% between 5 and 10 min of analysis. The sample containing 0.05% v/v suspended solids also reached its maximum transmittance value, although in a longer time interval, approximately between 15 and 20 min.
The results presented in Figure 5 demonstrate the temporal stability of the EG/H2O solution and the precipitation tendency of the evaluated nanofluids. Furthermore, it is evident that the nanofluid with 0.05% v/v demonstrates a slower sedimentation rate than those with 0.5% and 0.25% v/v, indicating enhanced stability in suspension during the initial minutes of the experiment.
The application of mechanical waves to materials generates distinct patterns. Such phenomena are known as Faraday instability and Chladni figures in the context of liquid and metallic plates
Figure 6 illustrates the vibration patterns of different sample compositions subjected to mechanical waves. The samples include (a) pure ethylene glycol, (b) an ethylene glycol/water mixture, and (c) an ethylene glycol/water-based nanofluid containing 0.5% v/v Fe₃O₄ nanoparticles. The experiment used a mechanical wave generator loudspeaker configured at 200 Hz and 45 dB. Due to the high viscosity of pure ethylene glycol (Figure 6a), this frequency was insufficient to disrupt the surface equilibrium, resulting in the absence of a visible pattern. However, in Figures 6b and 6c, where the base fluid is a mixture of ethylene glycol and water, the reduction in viscosity facilitated the appearance of the Faraday instability, resulting in the formation of distinct surface patterns. This phenomenon was further influenced by Fe₃O₄ nanoparticles in the nanofluid.
The excitation of the fluid depends on its composition; a decrease in the surface excitation pattern is observed in the sample with nanofluid, due to the addition of nanoparticles with respect to the ethylene glycol/water fluid base, as can be seen in Figures 5b, c). The relationship between the excitation source and the vessel must be a fixed junction so that the mechanical wave can be transmitted to the fluid, which is the only one free to move. On the other hand, generating mechanical waves also introduces the presence of a magnetic field during its operation. This produces clusters of nanoparticles due to their magnetization, leading to particle aggregation and sedimentation, which negatively affects radiation absorption and, consequently, energy transformation.
Figure 7 illustrates the temporal thermal behavior of the evaluated samples, demonstrating the thermal performance of the two thermocouples at varying heights, as outlined in Section 2.3. Expected during agitation of the fluid, an increase in the bottom part and a decrease in the top part to homogenize the temperature of the sample.
If a fluid does not exhibit variations in its optical properties, its heating will remain homogeneous regardless of its thickness. However, if the fluid is slightly transparent in the visible spectrum, the upper layers absorb more radiation and reach higher temperatures.
In a stratified fluid, agitation generates currents that promote particle movement, allowing all particles to reach the upper layers and receive, on average, the same amount of radiation. This resulted in a more uniform heat distribution throughout the fluid volume.
Based on these ideas, the results in the figure support this explanation. Figure 7(a) shows that ethylene glycol reached similar temperatures at both measurement positions. Additionally, agitating the sample at 200 Hz reduced the temperature difference. These observations indicate that ethylene glycol acts as a transparent fluid and achieves homogenization during heating, with the applied agitation further enhancing this process.
In Figures (b-d), the upper and lower temperatures differ in all cases, indicating a stratification process. The presence of nanoparticles alters the fluid’s optical properties, having this effect. Additionally, the final temperature was varied by the nanoparticle volume fraction.
Regarding the effect of agitation, Figure 7(b) shows that the agitated fluid reaches a higher temperature than the reference sample. In Figure 7(c), both tests yield similar results. In Figure 7(d), the top temperature of the agitated sample is lower than that of the reference sample, suggesting reduced stratification after 5 min. However, particle precipitation, which increases over time and is particularly relevant for samples with a 0.5-volume fraction, could also explain this effect. Finally, the applied agitation frequency did not significantly improve the temperature homogenization.
Figure 8 shows the evolution of the temperature difference (ΔT) between the upper and lower parts of the samples over time, considering the presence and absence of an excitation frequency of 200 Hz. In general, the temperature difference reaches a maximum around 3-4 minutes and then gradually decreases, indicating a tendency toward thermal equilibrium. Nanofluids with Fe₃O₄ concentrations show higher temperature differences compared to the base fluid (EG/H2O), with the 0.5% v/v sample showing the highest ΔT. Furthermore, the application of the 200 Hz frequency tends to reduce the temperature difference in all cases, suggesting that mechanical excitation promotes thermal homogenization within the fluid.
The sample that exhibited minimal thermal stratification when using the loudspeaker was ethylene glycol-water, a phenomenon that persisted throughout the evaluation period. In the 0.05% concentration, the effect of the loudspeaker on thermal stratification was noticeable after four minutes. In the 0.25% sample, thermal behavior exhibited a high degree of similarity under both conditions, with and without the loudspeaker. The 0.5% concentration exhibited the most pronounced stratification in the absence of a loudspeaker. The thermal difference among the samples decreases over time.
The 0.5% v/v sample showed the most pronounced thermal stratification without the loudspeaker, reaching the highest temperature difference at the start of the test. However, applying acoustic excitation at 200 Hz gradually reduced stratification throughout the experiment, except at minute three, where the thermal change remained similar. These findings suggest that acoustic excitation directly influences thermal stratification, with stronger effects appearing in the 0.0% and 0.05% v/v samples.
Figure 9a shows the evolution of the Specific Absorption Rate (SAR) over time for different concentrations of Fe₃O₄ nanoparticles (0.05%, 0.25%, and 0.5% v/v) under conditions with and without acoustic excitation (200 Hz). The y-axis represents the SAR values (W/kgFe₃O₄), while the x-axis corresponds to the time in minutes. The results show that the nanoparticle concentration significantly affects the thermal behavior of nanofluids. In particular, the lowest volume fraction (0.05% v/v) exhibited the highest SAR values, which is consistent with the definition of SAR as the energy absorbed per unit mass of nanoparticles. As the total mass of solids decreases, the energy absorbed per particle is relatively higher. Conversely, as the concentration increases (0.25% and 0.5% v/v), the specific yield decreases, resulting in a decrease in SAR values, as shown in Figure 10a. In addition, the data show that SAR tends to be higher in the absence of acoustic excitation, further supporting the observation that sound waves do not enhance energy absorption under the conditions studied and may even contribute to a reduction in SAR.
Figure 9b shows the Specific Absorption Rate (SAR) for different concentrations of Fe₃O₄ nanoparticles (0.05%, 0.25% and 0.5% v/v) under two conditions: without acoustic excitation (orange) and with acoustic excitation (blue). The results show that for all concentrations evaluated, the SAR is higher without acoustic excitation, with the most notable difference observed at 0.05% v/v. As the nanoparticle concentration increased (0.25% and 0.5% v/v), the SAR values decreased under both conditions, and the effect of acoustic excitation became even less pronounced. Although theoretical models suggest that sound waves enhance nanoparticle dispersion and heat transfer, the experimental results show the opposite effect under the specific frequency and amplitude conditions investigated in this study. This suggests that in this setup, acoustic excitation does not improve energy absorption efficiency and may even contribute to the reduction in SAR.
The Figure 10 shows the evolution of the SER (Signal Enhancement Ratio) over time (in minutes) for different Fe₃O₄ concentrations (0.05% v/v, 0.25% v/v, and 0.5% v/v) under with and without acoustic excitation at 200 Hz. The y-axis represents the SER value in dimensionless units (di), and the x-axis represents the elapsed time.
The results showed that 0.5% v/v concentration had the highest SER values, with a decreasing trend over time. Conversely, this concentration provided the optimal SER regardless of the presence or absence of acoustic excitation. In contrast, the 0.05% and 0.25% v/v concentrations showed more stable values, remaining close to one, with slight variations. Specifically, for the 0.25% v/v concentration under acoustic excitation, the SER remained close to unity throughout the evaluated time. In addition, for the 0.05% v/v concentration, no differences in SER values were observed between the conditions with and without the loudspeaker.
Furthermore, the presence of acoustic excitation at the lowest concentration (0.05% v/v - 200 Hz) did not seem to significantly increase the SER compared with the non-excitation condition. Taken together, these results suggest that a higher nanoparticle concentration initially promotes a higher SER, but over time, it tends to stabilize.
In the overall experiment, low-frequency acoustic excitation did not yield a consistent improvement in thermal efficiency, so a global performance increase cannot be claimed. However, an early advantage was observed: during the first 5 minutes, the excited samples showed a higher initial SAR. Therefore, it is advisable to assess efficiency using time-windowed metrics that capture time-dependent effects.
This work presents a simplified and replicable experimental setup that integrates optical stability and thermal performance under visible and infrared irradiation. This setup enables simultaneous evaluation of stratification and efficiency during audible excitation. The results indicate that excitation reduces stratification and facilitates thermal homogenization, with a dependence on concentration, though without consistently leading to overall improvements.
While the study demonstrates the viability of the approach, there are limitations that can be addressed: the use of a single frequency-amplitude set, along with a confined geometry, is a contributing factor. Additionally, colloidal stability was found to be restricted, which has the potential to influence efficiency estimates. Similarly, the presence of a magnet in the loudspeaker could impact measurements due to attraction or aggregation effects. These constraints can be mitigated by using the same setup with a systematic sweep of frequency and amplitude, comparing cell vs. flow configurations, and using nanofluids with greater temporal stability or alternative compositions. Ideally, the loudspeaker would be replaced with a piezoelectric actuator to more comprehensively determine how these factors affect thermal performance.
In contrast with other reports, which demonstrate significant improvements in transfer and system efficiency through the use of rotating magnetic fields or ultrasound in regimes with strong cavitation
The transmittance results in the visible spectrum demonstrate that formulations with 0.25% and 0.5% v/v concentrations of Fe3O4 exhibit rapid sedimentation, reaching 100% transmittance in less than 10 min, indicating a significant loss of stability. Conversely, the sample with 0.05% v/v exhibited enhanced resistance to sedimentation, retaining its opacity for a longer period.
The specific absorption rate (SAR) analysis indicated that the formulation with 0.05% v/v Fe3O4 exhibited the highest thermal energy conversion efficiency, whereas at higher concentrations, a decrease in the relative efficiency was observed. Furthermore, the application of acoustic waves at 200 Hz and 45 dB did not significantly improve the temperature reached by the fluid, suggesting that the effectiveness of mechanical excitation depends on the concentration of nanoparticles and the properties of the system. These findings highlight the importance of adjusting excitation conditions to optimize heat transfer in nanofluids used in solar collection systems.
Future studies should use nanofluids with greater stability and minimal variation in viscosity with temperature to isolate and evaluate the effect of acoustic excitation on thermal performance.
This work was also financed by the project “RC-2022-0766 - MINCIENCIAS - Diseño de un sistema de calentamiento complementario por inducción magnética termosolar, con uso nanosuspensiones desarrolladas a partir de materiales de procesamiento minero - H:51691”. In addition, this research was supported by the BEDA program of the Universidad Nacional de Colombia – Sede Medellín.
The authors declare that they have no conflict of interest.